Geschmierte Nylonqualitäten: PTFE, MoS₂ und ölgefüllte Optionen für Verschleißanwendungen

lubricated-nylon-ptfe-mos2-oil-filled-grades
lubricated nylon ptfe mos2 oil filled grades

Why Lubricate Nylon?

Nylon’s natural surface properties include a relatively low coefficient of friction compared to many engineering plastics—but it’s not inherently self-lubricating. In moving-part applications like gears, bearings, slides, and cams, unlubricated nylon can experience accelerated wear, frictional heating, and stick-slip behavior. Lubricated nylon grades solve this by incorporating solid or liquid lubricants directly into the polymer matrix, creating parts that run smoothly for millions of cycles without external lubrication.

The lubricant additives work by forming a transfer film on the mating surface. As the nylon part moves, microscopic lubricant particles are released, coating both the nylon surface and the opposing metal or plastic surface. This film reduces the coefficient of friction from 0.35–0.40 (unmodified nylon on steel) down to 0.10–0.20, depending on the lubricant type and loading.

The Three Main Lubricant Types

Lubricant Typical Loading COF (vs Steel) Beste Bewerbung
PTFE (Teflon) 10–20% 0.10–0.18 High-speed bearings, low-load slides
MoS₂ (Molybdenum Disulfide) 1–5% 0.12–0.20 High-load gears, thrust washers
Oil-filled 2–8% 0.08–0.15 Precision bearings, low-noise applications

PTFE-Filled Nylon

PTFE (polytetrafluoroethylene) is the most common solid lubricant for nylon. With a coefficient of friction as low as 0.04 in its pure form, PTFE particles dispersed throughout nylon create an extremely low-friction surface. PTFE-filled nylons are ideal for high-speed, low-to-moderate load applications where continuous sliding motion is required.

The limitation: PTFE reduces mechanical strength by 10–20% and increases cost. It also doesn’t perform as well as MoS₂ under very high contact pressures.

MoS₂-Filled Nylon

Molybdenum disulfide has a layered crystal structure similar to graphite—sheets that easily slide past each other. This makes it exceptional under high contact pressures where PTFE would be squeezed out. MoS₂-filled nylon is the go-to choice for gears, cams, and thrust washers operating under significant load.

MoS₂ also increases nylon’s crystallinity slightly, which can improve strength and stiffness—unlike PTFE which weakens the matrix. The dark gray/black color can be a consideration for visible parts.

Oil-Filled Nylon

Oil-filled nylons incorporate lubricating oil directly into the polymer during compounding. During operation, the oil slowly migrates to the surface, providing continuous lubrication throughout the part’s life. This “self-replenishing” characteristic makes oil-filled nylon excellent for sealed applications where relubrication is impossible.

Common oils include silicone, mineral oil, and synthetic hydrocarbon oils. The oil content is precisely controlled to avoid excessive migration that could contaminate surrounding components.

Content image
Illustration des Inhalts

Wear Rate Comparison

Nylon-Sorte K-Factor (×10⁻⁸ mm³/N·m) PV Limit (MPa·m/s) Service Temp Range
PA6, ungefüllt 40–80 0.09–0.12 -30°C to 85°C
PA6 + 15% PTFE 5–12 0.15–0.25 -40°C to 100°C
PA6 + MoS₂ 8–15 0.20–0.35 -30°C to 95°C
PA66 + Aramid + PTFE 2–5 0.35–0.50 -40°C to 120°C

Design Guidelines for Lubricated Nylon Parts

  • Surface finish of the mating part: Aim for 0.2–0.4 μm Ra on the steel/opposing surface. Rougher surfaces accelerate wear.
  • Clearance: Allow 0.3–0.5% of the bearing diameter for thermal expansion and water absorption swell.
  • Wandstärke: Maintain uniform wall thickness to avoid warpage that creates uneven wear patterns.
  • Running-in period: Expect higher friction during the first 500–1000 cycles as the transfer film establishes.
  • Combination with glass fiber: Adding glass fiber to lubricated nylon improves load capacity but increases wear on the mating surface. Use hardened steel (58+ HRC) for mating parts.

Warum sollten Sie Nylon-Kunststoff für Ihren Bedarf an technischen Kunststoffen wählen?

  • 300+ Spritzgießmaschinen von 50T bis 2000T
  • Mehr als 10.000 Teile pro Tag Produktionskapazität
  • ±0,02mm Genauigkeit Toleranz für alle Materialien
  • MOQ nur 1 Stück für das Prototyping; skalierbar auf Millionen
  • 24-Stunden-Quotierung, 3-15 Tage Vorlaufzeit
  • ✅ ISO 9001 zertifiziertes Qualitätsmanagementsystem

Erhalten Sie ein Angebot innerhalb von 24 Stunden →

Verwandte Artikel

FAQ

How do you know whether Lubricated Nylon Grades: PTFE, MoS₂ and Oil-Filled Options for Wear Applications fits a part?

Lubricated Nylon Grades: PTFE, MoS₂ and Oil-Filled Options for Wear Applications fits a part when its load capacity, temperature range, moisture exposure, wear behavior, and processing method match the real service conditions.

What properties should be checked for Lubricated Nylon Grades: PTFE, MoS₂ and Oil-Filled Options for Wear Applications?

Prüfen Sie Festigkeit, Steifigkeit, Schlagfestigkeit, Hitzebeständigkeit, Feuchtigkeitsaufnahme, Formstabilität, Reibung, Verschleiß und chemische Verträglichkeit.

What is the biggest selection risk for Lubricated Nylon Grades: PTFE, MoS₂ and Oil-Filled Options for Wear Applications?

Das größte Risiko besteht darin, sich auf einen Wert aus dem Datenblatt zu verlassen, ohne die tatsächlichen Umgebungsbedingungen, das Verarbeitungsverfahren, die Bauteilgeometrie und die langfristige Nutzung zu berücksichtigen.

When should Lubricated Nylon Grades: PTFE, MoS₂ and Oil-Filled Options for Wear Applications be tested before production?

Prüfungen werden empfohlen, wenn das Bauteil Belastungen, Hitze, Chemikalien, Feuchtigkeit, engen Toleranzen, gesetzlichen Anforderungen oder einer neuen Betriebsumgebung ausgesetzt ist.

Erzählen Sie uns etwas über Ihr Bauteil

Dieses Feld ist erforderlich.
Dieses Feld ist erforderlich.
Dieses Feld ist erforderlich.
Dieses Feld ist erforderlich.
Dieses Feld ist erforderlich.

Weiterführende Lektüre

Nach oben blättern